One Number Is Not a Curve: Full Pressure-Sweep Test Data for Our GSF130-030 Graphene Thermal Pad

Date:2026-11-26 

When you ask us for a thermal pad's resistance, the honest answer is never one number. It's a number with a pressure attached. Change the clamp force and the interface changes with it — sometimes dramatically. If the pressure in our lab report doesn't match the pressure your structure can actually deliver, the datasheet value is trivia, not data.

So for GSF130-030, our 0.3 mm graphene thermal pad, we did the boring but necessary thing: we swept the pressure from 10 to 100 psi and recorded thermal resistance and compression rate at every step. This article gives you the specimen details, the test conditions, every measured point, the TDS context — and the boundaries of what the data means. If you design heat paths or buy thermal interface materials, this is the shape of evidence worth asking any supplier for.

 

GSF130-030 Graphene Thermal pad test

 

1. A Single 50-psi Value can't Describe Your Interface

Interface thermal resistance is roughly the pad's bulk resistance plus two contact resistances, one on each face. Pressure is what collapses microscopic gaps and drives the contact terms down — which is why every serious resistance figure carries a test pressure next to it. Our TDS quotes ≤0.06 °C·cm²/W at 50 psi, and that's a fair statement of the product. It just isn't the whole story.

Here's the question your assembly actually asks: what does the pad do at my pressure? A light screw pattern over a large chip, a spring clip with modest preload, a housing that must not bow — each delivers a different clamp force, and none of them owes the datasheet 50 psi. A pressure sweep answers that question directly. It also exposes something a single point hides: where more pressure stops paying back.

That second curve, compression rate, matters just as much. Compression is the price you pay for contact — in component stress, board bending, and how much of your design gap the pad consumes. Measuring both curves on the same specimen lets us talk about cost and benefit in the same units as your mechanical budget.

 

2. The Specimen, the Instruments, and the Conditions

Everything below comes from our GSF130-030 test report and the product TDS. We've reproduced the numbers without rounding or selection.

 

Sheen Technology test Laboratory

Figure 1. Sheen Technology’s specialized testing laboratory is used to evaluate the performance parameters of thermal interface materials.

 

ItemValue
SpecimenGraphene thermal pad, model GSF130-030
Nominal thickness0.3 ± 0.03mm
Initial measured thickness0.276 mm (compression-rate specimen)
Test date23 October 2026
LocationSheen quality inspection laboratory
Thermal resistance10–100 psi, LONG WIN thermal tester LW-9389, per ASTM D5470
Compression rate10–100 psi, universal electronic testing machine, per ASTM F36

Table 1. Specimen and test setup, from the GSF130-030 test report. ASTM F36 is the standard compressibility-and-recovery method for gasket-type materials — a fitting frame for a pad asked to conform under clamp load.

 

Sheen Technology Graphene Thermal pad

Figure 2. GSF130-030 product photo.

 

GSF130-030 is built from graphene as the core conductive filler, directionally aligned and laminated to form a through-thickness heat path. Its TDS reads as follows:

 

PropertyGSF130-030Test standard
Thermal conductivity130 W/m·KASTM E1461
Thermal resistance @50 psi≤0.06 °C·cm²/WASTM D5470
Operating temperature−40 to 150 °C—
Rebound rate≥90%—
Tensile strength (orientation direction)≥0.05 MPaASTM D412
Density0.3–0.7 g/cm³ASTM D792
Oil bleeding rate≤3%—
FlammabilityV-0UL94
ColorBlackVisual
ComplianceRoHS 2.0, halogen, REACH—
Storage≤30 °C, ≤75% RH—
Shelf life12 months—

Table 2. GSF130-030 TDS parameters. Typical applications listed: semiconductor test, AI and autonomous-driving chips, optical modules, communications equipment, drones, humanoid robotics.

Two cautions before these numbers travel any further. The 130 W/m·K figure is a material-level conductivity measured per ASTM E1461 on the oriented structure — it is not a predicted temperature drop in your device, and it doesn't replace the interface-resistance data below. And the ≤0.06 °C·cm²/W ceiling is defined at 50 psi; keep that pressure tag attached to the number everywhere it goes.

 

3. Thermal Resistance Under Pressure: The Full Sweep

The resistance test ran on a LONG WIN LW-9389 thermal tester, referencing ASTM D5470, with roughly 70 W pushed through the specimen at each step. The hot side sat near 80 °C and the cold side near 79 °C in the instrument log. Here are all ten points, exactly as recorded:

 

PointPressure (psi)Power Q (W)R (°C/W)Resistance (°C·cm²/W)Resistance (°C·in²/W)
110.0272.230.0150.0960.015
220.0071.880.0110.0690.011
329.9871.450.0090.0560.009
439.9571.090.0080.0520.008
549.9570.730.0080.0490.008
659.9370.500.0070.0470.007
769.9870.280.0070.0460.007
879.9370.110.0070.0450.007
989.9369.970.0070.0430.007
1099.9569.810.0070.0420.007

Table 3. Instrument readings from the test report (LONG WIN LW-9389, ref. ASTM D5470). Hot-side temperature ≈80.0 °C, cold-side ≈79.0–79.6 °C across the run. R in °C/W is the whole-specimen reading; the two right columns are area-normalized. Don't mix the unit families — °C·cm²/W and °C·in²/W differ by a factor of about 6.45.

 

GSF130-030 Graphene Thermal pad Thermal resistance vs. pressure curve

Figure 3. Thermal resistance vs. pressure curve from the report data. The red dashed line represents the reference pressure corresponding to a thermal resistance of 0.06.

 

Read the curve the way your structure will experience it:

  • The low-pressure region is where the action is. From 10 to 50 psi, resistance falls from 0.096 to 0.049 °C·cm²/W — nearly a 49% improvement (calculated from the table). Every extra bit of clamp force in this band buys visible contact.
  • The TDS ceiling gets crossed on the way up. The specimen measured above the ≤0.06 spec at 10 and 20 psi (0.096 and 0.069), and first measured inside it at ~30 psi (0.056). That's not a contradiction — it's the definition. The spec is a 50-psi statement, and if your assembly lives below ~30 psi, the pad you receive will not perform like the headline number. At the spec point itself, ~50 psi, the specimen measured 0.049 — comfortably inside the ceiling.
  • Past 50 psi, the curve flattens. From 50 to 100 psi, resistance improves from 0.049 to 0.042 — a further 14%, and most of that arrives by 70 psi.

Neither endpoint is a "result" on its own. The curve is the result: this is how the interface responds across the whole pressure window a design might offer it.

 

4. Compression Under Pressure: What You Pay for Contact

The compression test ran on the same pressure grid per ASTM F36, on a specimen whose initial measured thickness was 0.276 mm:

 

Pressure (psi)Compression rate (%)Implied compressed thickness (mm, calculated)
107.20.256
2014.00.237
3021.00.218
4027.80.199
5034.70.180
6041.60.161
7048.60.142
8055.40.123
9062.30.104
10069.20.085

Table 4. Compression rate from the report (initial thickness 0.276 mm). The third column is our arithmetic — 0.276 × (1 − compression rate) — shown for gap planning, not a measured value. Note the specimen measured 0.276 mm against a 0.3 mm nominal; build your tolerance stack from measured, not nominal, thickness.

 

GSF130-030 compression rate VS pressure

Figure 4. Compression rate vs. pressure curve.

 

Two features stand out. First, the curve is close to linear — about 6.8–6.9 percentage points of compression per additional 10 psi across the whole range (calculated). The pad keeps squeezing at a steady rate; there's no plateau where it stiffens up and says "enough". Second, the absolute numbers are large: by 100 psi the specimen is compressed 69.2%, leaving barely a third of its initial thickness. That's useful information about the material's range — and a warning label, which we'll get to.

One practical note for your CAD gap: a nominal 0.3 mm pad is not a 0.3 mm spacer. At 50 psi this specimen worked at roughly 0.18 mm (calculated). If your gap model assumes the nominal thickness, your clamp load estimate will be wrong — in the dangerous direction.

 

5. Reading the Two Curves Together

Either curve alone invites a lazy conclusion. Together, they tell the story your design review needs:

  • 10 → 50 psi: compression rises from 7.2% to 34.7%, and resistance falls by ~49%. Contact is forming; pressure is paying off. This is the productive region.
  • 50 → 100 psi: compression doubles — from 34.7% to 69.2% — while resistance improves only another ~14%, from 0.049 to 0.042 °C·cm²/W. The pad keeps giving thickness, but the interface has little left to sell you. Doubling your clamp load past the spec point buys 0.007 °C·cm²/W.

The engineering translation is straightforward. If your structure can deliver around 30–50 psi, this pad works in its productive band and meets its published spec with room. If your structure delivers 10–20 psi, design against the measured 0.069–0.096 — not against the 50-psi headline, and not against the 100-psi tail. And if your plan was "just clamp it harder", the curves answer that too: beyond the spec point you're mostly spending stress, not buying conductivity.

Stress is a real budget, by the way. 69.2% compression is an extreme test point that tells you the material's envelope — it is not a design target. What the pad looks like after being held at that state, and how it recovers, are questions this report doesn't attempt to answer.

6. Boundaries Before You Design It in

We'd rather you trust this data for exactly what it is, so here are the fences:

  • Test conditions are not assembly instructions. The 10–100 psi sweep is a characterization grid. Nothing here tells you how hard to tighten anything.
  • Area-normalized resistance is not system resistance. The °C·cm²/W (or °C·in²/W) figures describe the interface under the instrument's conditions, not the °C/W of your assembled heat path. And never mix the two unit families without the ~6.45 conversion.
  • One specimen, one date, no batch recorded. The report covers a single test run on 23 October 2026. Production tolerances mean later batches can differ; the inspection report for your shipped batch is the one that governs.
  • No written conclusion. The report presents the data without a pass/fail statement. We've likewise made no claim beyond the numbers.
  • Ambient conditions for the compression test aren't stated.
  • Don't assume electrical insulation. The TDS lists no volume resistivity, breakdown voltage, or dielectric values, if your interface needs isolation. A soft, thin graphene-based pad is not an insulating layer by default.
  • Recovery is a separate question. The TDS rebound figure (≥90%) comes from its own short-duration test — it is not a reuse count, and it doesn't describe recovery after long holds at high compression. The "no pump-out" and "long-term stability" language in the TDS is product positioning; this report doesn't verify it. Aging, thermal cycling, and pump-out behavior need their own tests under your conditions.

None of these boundaries make the data less useful. They make it usable — because a design built on stated limits survives review, and one built on hoped-for limits survives until the first rework.

 

7. What to Send Us When You're Ready

The fastest path from these curves to your validation is a short list of inputs:

  • Gap range in the assembled state, including tolerances and board deformation
  • The pressure or total clamp force your structure actually delivers — screws, springs, clips, and how it's distributed
  • Operating temperature range and the heat load at the interface
  • Target interface resistance, and your preferred unit (°C·cm²/W or °C·in²/W)
  • Whether the interface needs electrical isolation, and any cleanliness limits (oil bleed, volatiles)
  • Expected rework frequency, so we can talk about recovery and reuse data rather than assume it

With those, we can point you to the right pressure band, the right thickness, and the right follow-up test — including anything on the list above. You may submit your requirements and get in touch with our team via the [sample request link]. And if your structure can't offer 50 psi, say so up front: that's exactly the conversation this data was published for.


A datasheet point is a promise made at someone else's pressure. A pressure sweep is the same promise written in your structure's language. We'd rather hand you the second one.

Sheen Thermal

Manufacturer of thermal interface materials and silicone foam for automotive electronics, energy storage, power electronics, communications and consumer electronics.

Certified

  • ISO 9001:2015
  • ISO 14001:2015
  • IATF 16949:2016

What we supply

  • Thermal conductivity Up to 130 W/m·K
  • Thickness 0.3–10.0 mm
  • Custom & samples Die-cut to drawing, 3–7 days
Request a Quote