Floating Cold Plates for 1.6T / 3.2T Modules: Holding Contact Through Every Insertion
Date:2026-11-25
Push a module into a cage and your hand feels one small click. Inside the cold plate, that click starts a negotiation that has to end the same way every single time — at the loosest slot, and after the thousandth swap. We want to walk you through that negotiation, because it is where most floating cold-plate designs quietly win or lose.

Figure 1. Pluggable optical module and chassis port.
One Insertion Splits the Problem in Two
Three things happen at once when the module goes in:
- The module slides along the wear-resistant layer. That face owns friction and wear.
- The floating cold plate steps aside along an axis perpendicular to insertion. It does not fight you; it makes room.
- Behind it, the pad compresses. Once the module seats, that same pad pushes back and holds the cold plate against the housing.
So the structure has already done something clever before we pick any material: it hands 'survive sliding' to one interface and 'hold contact' to another. The wear-resistant thermal material closest to the module takes the sliding contact; our CSF high-resilience pad between the floating plate and the liquid cold plate takes normal compression. That pad carries heat through its thickness, absorbs the assembly gap without demanding a perfect boss height, and supplies the preload that keeps the plate mated. Heat still crosses both faces in series, so a beautiful number on one side will never rescue the other. Air is the tenant we are trying to keep out — it pays no heat rent and refuses to move.

Figure 2. Side view of the floating cold plate. Along the heat-flow direction: module housing, wear-resistant thermal layer, floating cold plate, high-resilience thermal pad, liquid cold plate.
Look at Figure 2 once more. The back-side pad is the only part of this stack willing to give way and then come back for more. That makes one variable the centre of the whole design: how far that pad is compressed, and whether it stays compressed. But before we can choose that working point, we need the boundaries your project has to live inside.
The Boundaries Come Before the Material
At 1.6T and 3.2T, we ask for numbers before grades. Please bring us the module's sustained power, its short peak and how long that peak lasts, the shell temperature limit, and how load is shared across one row of ports. Two public references set the scale, not your specification:
- The Juniper 1.6T form-factor and thermal guidance lists a 16–43 W power range for the 1.6T family.
- OSFP MSA technical material projects some 1.6T coherent modules and future 3.2T datacenter modules in the 35–40 W class.
We treat those as design magnitudes only. Your project power comes from the module supplier's specification and your own measurement. Now put that power through a simple piece of arithmetic: if one segment of the heat path has an equivalent resistance of 0.20 °C/W, then 20, 30, and 40 W produce roughly 4, 6, and 8 °C of temperature difference. It is a steady-state example — internal heat distribution inside the module, coolant temperature rise, and flow sharing all move the real answer, and short power spikes have to be read as temperature versus time.
That arithmetic is why we refuse to optimise a single number. Three conditions have to hold at the same time:
- Shell temperature stays inside its limit.
- Steady-state preload survives heat and time.
- Full-travel insertion force stays within what a person — or a robot — can actually push.
More clamping force may improve one contact face while making insertion heavy and accelerating wear. Notice where all three conditions land: on how hard the pad is pressing, and for how long. Table 1 is how we turn the remaining risks into bench questions before any of that gets specified.
| Project challenge | How to judge it on the bench |
|---|---|
| Power surges and hot spots | Test steady-state full load and the specified power step separately. Log the highest shell temperature, time to peak, shell-temperature fall-back, and slot-to-slot temperature spread. |
| Insertion and tolerance | Measure minimum, nominal, and maximum gaps. Log full-travel insertion and extraction force, sliding behaviour of the wear layer, floating travel, and retention force. Judge each against the module and cage specifications. |
| Oil exudation and volatile deposition | After compression and thermal aging, inspect edge migration, oil traces, and deposits near the optical face. Match the material outgassing screen to an installed optical check. |
| Resistance drift after cycling | At the same module power, inlet temperature, flow, and measurement points, compare resistance, highest shell temperature, and slot spread across the first article and every cycle stage. |
| Conductive debris | Collect particles from the sliding face, cage, and connector area. Check size, count, source, and conductivity, then accept against the project's cleanliness and electrical criteria. |
Table 1. Five requirements, five test families. Fix the resistance-drift and particle criteria against the whole-system specification before you start the bench work.
Industry references in the source: Juniper 1.6T form factor and thermal design · OSFP MSA thermal management material.
With the boundaries written down, we can finally ask the useful question: where on the compression curve should this pad live?
Finding the Working Point
Our vertically oriented carbon fibers thermal pad line up along the pad thickness — the same direction heat travels from module to coolant. The CSF20-HR TDS lists 20 W/m·K through-thickness conductivity (ASTM D5470), Shore 00 hardness 45–55, and ≥80% recovery. Those are material properties. What your assembly does with them is a different story: post-compression thickness and the quality of both contact faces decide the resistance you actually get.
So we ran 2.0 mm specimens through three compression steps:

Figure 3. Bench curves at the same nominal thickness. Lines between points guide the choice of re-test conditions.
| 2.0 mm specimen | 20% compression | 30% compression | 40% compression |
|---|---|---|---|
| Peak stress, psi | 12.38 | 33.11 | 49.66 |
| After 10 min hold, psi | 5.08 | 13.41 | 16.80 |
| Thermal resistance, °C·in²/W | 0.189 | 0.180 | 0.196 |
| Converted, °C·cm²/W | 1.22 | 1.16 | 1.26 |
Table 2. Stress from the 2026-09-02 report, 25 × 25 × 2.0 mm specimens, five pieces per step.
- Going from 30% to 40% adds roughly half again to peak stress.
- In the resistance sweep, the reading moves from 0.180 to 0.196 °C·in²/W — about 9% higher.
- A separate fixed-pressure run recorded 0.277 °C·in²/W at 30 psi.
Our reading is simple: re-test around 30% first, then expand toward both tolerance ends. Two cautions travel with it. The reports do not give a measurement uncertainty large enough to judge whether that 9% difference is statistically significant, and that 0.277 value came from a different, fixed-pressure test — it is not a contradiction. Keep % and psi apart on your spec sheet: one says how far you pressed, the other how concentrated the load is; the two sets were recorded separately.
Using the 625 mm² compressed area of that specimen, 33.11 psi at 30% works out to roughly 143 N peak normal load and about 58 N after 10 minutes. Your real insertion force still has to be measured on the whole machine, because sliding friction, the lead-in ramp, and the connector all add resistance of their own.
Method reference from the source: ASTM D5470 thermal resistance testing.
Thirty percent, then — on day one. The problem is that your product does not live on day one. A module gets swapped minutes after the last one, and the assembly sits at temperature for years. Both of those pull the pad away from the point we just chose.
Does That Working Point Stay Put?
A working point is only useful if it survives. We look at two clocks: the short one between two swaps, and the long one inside an oven.
The short clock: after a hot swap
Two questions, not one. How much thickness comes back after unloading? And how much clamping force is still there after the module is re-installed? The first is unloaded recovery; the second is stress relaxation and assembly retention.

Figure 4. Unloading recovery of 25 × 25 × 1.7 mm specimens. Five pieces per step; the original report lists ASTM D575.
| Compression step | 5 min avg. recovery | 30 min avg. recovery | 2 h avg. recovery |
|---|---|---|---|
| 30% | 89.15% | 93.27% | 94.76% |
| 50% | 91.15% | 93.36% | 94.25% |
| 80% | 66.67% | 90.58% | 93.11% |
Table 3. Recovery = recovered displacement ÷ original compressed displacement. The 80% step is an extreme test condition, and its 5-minute average is only 66.67%. If your tolerance stack over-compresses a single slot, check short-time recovery and re-installed contact there first.
The long clock: after 2,000 hours
We aged 2.0 mm CSF20-HR at 125 °C and 150 °C for 2,000 hours each, then re-measured the same three things a designer actually depends on:
| 2.0 mm CSF20-HR | Initial | After 125 °C | After 150 °C |
|---|---|---|---|
| Resistance @30 psi, °C·in²/W | 0.304 | 0.241 | 0.219 |
| Short-term recovery | 92.2% | 98.01% | 98.01% |
| Hardness, Shore 00 | 47 | 55 | 59 |
Table 4. Both temperature groups ran 2,000 h. Recovery condition: 50% compression held 30 min, then unloaded for 30 min. The report notes no visible cracking or chalking.
One number deserves your attention: hardness in the 150 °C group moves from Shore 00 47 to 59. A harder pad changes both load and insertion feel, so clamping force, insertion force, and shell temperature all deserve a re-measure on real hardware. Oven data earns a material a seat at the table; it does not sign off a whole system. Constant-compression aging, hot insertion, and post-cycle resistance each need validation on your own structure.
Both clocks say the same thing: preload drifts. The working point has to be chosen for its worst state, not its first one. And there is a second kind of spread we have not touched yet — the six slots in one row do not even start at the same compression.
Six Slots, Six Different Gaps
Our original application record covers two customers, and we want to be precise about what that means. Y works on datacenter liquid-cooling systems; S builds liquid-cooling modules. Both took part in the cold-plate structure and thermal design, and the material went through the system maker's validation together with the cold plate before entering volume production. The disclosed reference duty is 20 W per port, six positions on a top cold plate, 32 ports on a 1U platform.

Figure 5. Sheen project photos. Left: six-position cold plate and cover plate. Right: detail of metal parts mated with the thermal pad.
The stack uses a floating copper block, a phase-change material, a wear-resistant stainless steel sheet, and a high-resilience carbon fiber pad. A groove controls the copper block's lateral position while the pad compresses along its thickness. At 20 W per port over a nominal 6 cm² heat-transfer area, nominal heat flux is about 3.3 W/cm². A one-dimensional estimate over that area gives a temperature-rise budget of roughly 4.2–4.6 °C from the module shell to the groove base — useful for allocating your thermal budget and placing thermocouples. The real delta-T is measured on the whole machine.
Now put the working point next to a real tolerance stack. The nominal gap hides both risks:
| Nominal pad thickness | Tightest 1.1 mm | Nominal 1.4 mm | Loosest 1.7 mm |
|---|---|---|---|
| 1.7 mm | 35.3% | 17.6% | 0% |
| 2.0 mm | 45.0% | 30.0% | 15.0% |
Table 5. Tolerance example calculated from nominal free thickness. Real results also depend on pad thickness tolerance, boss and module-shell flatness, and floating travel.
- A 1.7 mm pad may have no preload at all in the loosest slot.
- A 2.0 mm pad in the tightest slot needs a check of peak load, insertion force, and available travel.
- For a production design you can evaluate adjusting boss height, binning by slot, or changing the effective compressed area — then re-measure in the real assembled state.
So thickness is not chosen at the nominal gap. It is chosen at the two ends — the loosest slot that still needs preload and the tightest slot that still allows insertion. The published case describes application and production status only; whole-system cycle counts and before/after resistance differences have to be confirmed against your own project data. We will not turn a case record into a lifetime promise.
Once both ends are bounded, the grade question becomes much smaller.
Turning That Rule Into a Grade
Start from the expected compression window, then use the stress curve to estimate face pressure — especially if the floating block has to stay preloaded in the loosest slot. If your thermal budget is tight, compare the mechanically acceptable candidates at the same post-compression thickness and the same assembly boundaries. We recommend CSF20-HR for the first round, because it is the one grade where we can cross-check 1.5 / 2.0 mm bench resistance, 2.0 mm stress data, and 1.7 mm recovery data against each other.
| Model | Through-thickness conductivity | Shore 00 / recovery | TDS resistance and condition |
|---|---|---|---|
| CSF10-HR | 10 W/m·K | 45–55 / ≥80% | ≤0.40, 2.0 mm / 30 psi |
| CSF15-HR | 15 W/m·K | 50–60 / ≥90% | ≤0.35, 2.0 mm / 30 psi |
| CSF20-HR | 20 W/m·K | 45–55 / ≥80% | ≤0.33, 2.0 mm / 30 psi |
| CSF25 | 25 ± 2.5 W/m·K | 60–70 / not listed in TDS | 0.11 ± 0.02, 1.0 mm / 10–15% compression |
Table 6. From each grade's ASTM D5470 data. Recovery follows each TDS's own definition — align compression ratio, hold time, and recovery time before comparing.
- Use CSF10-HR or CSF15-HR as different conductivity control points. Real softness, stress, and retention force come from your own sample tests.
- CSF25 is worth evaluating for thin gaps and tight thermal budgets.
- For a floating cold-plate back-side pad, confirm stress at the target compression, unloaded recovery, and long-term retention force.
One more reminder that a TDS number wears a lab coat. That settles the back-side pad. It does not settle the sliding face, which is the other half of the split we started with.
The Other Half, and How We Prove It

Figure 6. Stack schematic. The wear-resistant thermal layer sits on the sliding contact face of the floating cold plate; the elastic pad sits behind it.
The back-side pad should never be asked to survive sliding. Select the wear-resistant layer separately: either a thermally conductive composite with a metal wear face, or a wear-resistant surface layer that has already been validated. If you build it on a phase-change base material, re-test the finished composite's resistance, insertion force, wear behaviour, and exudation — the base material's numbers no longer describe the finished part.
Then prove both halves together with an A/B plan. Fix one wear layer on the cold-plate bench and compare two CSF pad options; once the back-side pad is chosen, hold it fixed and compare wear layers. When insertion force or resistance moves, you can then tell whether the sliding face wore down or the back-side pad's clamping force changed.
| Validation stage | What to record | What to judge it against |
|---|---|---|
| Initial assembly | Measure gap, post-compression thickness, floating travel, and initial plus retained face pressure at tolerance extremes. Log full-travel insertion force at real machine speed. | The loosest slot still makes contact; the tightest slot stays inside load and insertion-force limits. |
| Load and cycling | Run cold and hot insertions plus power steps as the customer specifies. Re-measure resistance and every slot's shell temperature in stages, then re-test after cycling at the same temperature, flow, and measurement points. | Check resistance drift with (Rₙ − R₀) / R₀, where R₀ is the initial value and Rₙ is the post-cycle value. Also review peak shell temperature and insertion-force curves. |
| Cleanliness and reliability | Inspect sliding-face debris, die-cut pad edges, the cage, and connectors separately. Add oil-migration checks, deposition witness plates, particle conductivity, and constant-compression aging as the project requires. | Accept against the customer's cleanliness, optical, and electrical criteria; record sampling range and detection limits. |
Table 7. Recommended A/B validation flow. Cycle count, temperature range, acceptable resistance drift, and particle limits are defined by the whole-system project.
Two risks are easy to conflate, so we keep them apart:
- Conductive debris starts as a structural decision. Keep the carbon-fiber pad inside the back-side groove, away from the module's sliding path. After the material and die-cut plan are fixed, inspect edge residue, clamping, and friction marks. Any claim of 'no conductive debris' only means what was verified under agreed conditions and detection limits.
- Low oil exudation and low volatiles need different tests. Exudation is migration under compression, temperature, and time. Volatiles can be pre-screened with ASTM E595 vacuum outgassing — but whether your optical face is actually affected needs a witness plate or a whole-system optical metric.
Method references from the source: ASTM E595 vacuum outgassing screening · ASTM D5470 thermal resistance testing.
At this point the material choice has become a set of records: gap, load, resistance, recovery, and cleanliness, all tied to one agreed test condition. That is what survives a design review, and what your next platform can reuse.
Start From Your Drawing Tolerances
Send us the module outline and rated / peak power, the boss length and width, the minimum / nominal / maximum assembly gap, the allowed insertion force, and your target cycle count. With those in hand we can discuss CSF standard or custom thicknesses, die-cut dimensions, and separate validation plans for the back-side pad and the wear layer.
We would rather see your tolerance stack than your target conductivity number. The first one tells us whether the pad will still be holding contact at the loosest slot on its thousandth insertion — which is exactly where this conversation started.
Request CSF samples and Sheen material data: www.sheenthermal.com/feedback.html
Sheen Thermal
Dongguan Sheen Electronic Technology Co., Ltd · Founded in 2008
Manufacturer of thermal interface materials and silicone foam for automotive electronics, energy storage, power electronics, communications and consumer electronics.
Certified
- ISO 9001:2015
- ISO 14001:2015
- IATF 16949:2016
What we supply
- Thermal conductivity Up to 130 W/m·K
- Thickness 0.3–10.0 mm
- Custom & samples Die-cut to drawing, 3–7 days